Pinus strobus

 

 

click here for the page in Engilsh units of measure

this page uses metric units of measure

 

Family: L. Pinaceae

 

 

 

 

 

 

click to print or download the file in .pdf format

 

Eastern White Pine

 

 

 

 

The genus Pinus is composed of about 100 species native to temperate and tropical regions of the world. Wood of pine can be separated microscopically into the white, red and yellow pine groups. The word pinus is the classical Latin name and strobus is the Latin name for pine cone, from the Greek strobos (whirling around) and strobilos (pine cone). The species Pinus stobus is composed of two varieties; the typical Eastern White Pine (Pinus strobus var. strobus L.) and Chiapas White Pine (Pinus strobus var. chiapensis Martinez [P. chiapensis (Martinez) Andresen]), native to the mountains of southern Mexico and Guatemala.

Other Common Names: American white pine, American yellow pine, apple pine, ayacahuite vidriosa, balsam pine, bor vajmutov, borovice tuha, Canadian white pine, Canadian yellow pine, chiapas pine, chiapas white pine, Chiapas-pijn, chiapas-tall, cork pine, eastern pine, eastern white pine, kahikatea, Minnesota soft white pine, Minnesota white pine, New England pine, northern pine, northern white pine, Ottawa pine, Ottowa white pine, pattern pine, pin baliveau, pin blanc, pin blanc canadian, pin de Chiapas, pin du lord, pin jaune, pin potiron, pin Weymouth, pino ayacahuite, pino canadiense, pino di Chiapas, pino stobo, pino Weymouth, pumpkin pine, Quebec pine, Quebec yellow pine, sapling pine, seidenkiefer, silver pine, simafenyo, soft pine, soft cork white pine, soft pine, soft white pine, sosny wejmutka, spruce pine, strobe, strobo, strobus, tonawanda pine, Weymouth pine, Weymouth-pijn, Weymouth-pijn, weymouthpijn, Weymouths kiefer, weymouthsden, weymouthsfohre, weymouthskiefer, Weymouth-tall, weymouth-tall, Weymut-tall, weymut-tall, white pine, white soft pine, Wisconsin white pine, yellow pine.

Distribution: Eastern white pine is native to North America from Newfoundland, the Anticosti Islands and the Gaspe’ Peninsula of Quebec, west to central and western Ontario and extreme southeast Manitoba, south to southeastern Minnesota and northeastern Iowa, east to northern Illinois, Ohio, Pennsylvania and New Jersey and south to northern Georgia and northwest South Carolina. It is also locally distributed in western Kentucky, western Tennessee and Delaware.

The Tree: Eastern white pine grows to heights of 100 feet with a diameter of 3 to 6 feet. Historically, it has grown to heights of 200 feet with diameters of 6 feet. Current national champions are taller than 140 feet. Most of the large trees had been logged prior to the late 1800’s.

General Wood Characteristics: The heartwood of Eastern white pine is a light brown, sometimes with a reddish tinge, turning darker on exposure. The sapwood is white, tinged with yellow. It has a uniform texture, is easily worked with tools, shrinks little, easily kiln dried, is straight grained and has a high ability to stay in place. It has medium strength values, is easily worked and take stains, glue and finishes well. It also has good nail-holding ability. It is light weight, moderately soft, moderately weak, not stiff, and low in shock resistance.

 

 

Mechanical Properties (2-inch standard)

 

 

 

 

Compression

 

 

 

 

Specific

gravity

MOE

GPa

MOR

MPa

Parallel

MPa

Perpendicular

MPa

WMLa

Kj/m3

Hardness

N

Shear

MPa

Green

0.34

6.83

33.8

16.8

1.52

35.8

1290

4.69

Dry

0.37

8.55

59.3

33.1

3.03

46.9

1690

6.20

aWML = Work to maximum load.

Reference (56).

 

Drying and Shrinkage

Type of shrinkage

Percentage of shrinkage
(green to final moisture content)

0% MC

6% MC

20% MC

Tangential

6.1

4.8

2.0

Radial

2.1

1.8

0.8

8.2

6.6

2.7

3.3

References: (56, 178, 192).

Kiln Drying Schedulesa

 

Conventional temperature/moisture content-controlled schedulesa


Condition

4/4, 5/4
stock

6/4 stock

8/4
stock

10/4
stock

12/4
stock

British schedule
4/4 stock

Standard

T9-C5

NA

T9-C4

NA

NA

NA

Antibrown-Stain

276

NA

277

NA

278

NA

aReference (28, 185).

 

Conventional temperature/time-controlled schedulesa

 

Lower grades

Upper grades


Condition

4/4, 5/4 stock

6/4 stock

8/4 stock

4/4, 5/4 stock

6/4 stock

8/4 stock

12/4, 16/4 stock

Standard

308

NA

309

NA

NA

NA

NA

aReferences (28, 185).

Working Properties: It is easily worked with tools, is straight grained and has a high ability to stay in place. It takes stains, glue and finishes well. It also has good nail-holding ability.

Durability: Eastern white pine is rated as moderately resistant to heartwood decay (12).

Preservation: The heartwood is rated as moderately resistant to preservative treatment, while the sapwood is permeable (4).

Uses: The bark is used to produce white pine tar, an antiseptic and expectorant. The wood is used for furniture, patterns, matches, boxes, sashes, doors, trim, caskets and toys. The tree is a popular Christmas tree.

Toxicity: In general, working with pine wood may cause dermatitis, allergic bronchial asthma or rhinitis in some individuals (3, 7 & 14).

Additional Reading and References Cited (in parentheses)

1. Betts, H. S. Eastern White Pine (Pinus strobus). Washington, DC, USA: USDA Forest Service, 301226-54; 1954.

2. Boone, R. S.; Kozlik, C. J.; Bois, P. J., and Wengert, E. M. Dry kiln schedules for commercial woods - temperate and tropical. Madison, WI: USDA Forest Service, FPL-GTR-57; 1988.

3. Hausen, B. M. Woods injurious to human health. A manual. New York, NY: Walter de Gruyter; 1981.

4. Henderson, F. Y. A handbook of softwoods. London: HMSO; 1977.

5. Hyam, R. and Pankhurst, R. Plant and their names. A concise dictionary. Oxford, UK: Oxford University Press; 1995.

6. Little, Jr. E. L. Checklist of United States Trees (Native and Naturalized). Washington, D.C.: U.S. Government Printing Office, USDA, Forest Service, Agriculture Handbook No. 541; 1979.

7. Mitchell, J. and Rook, A. Botanical dermatology: plants and plant products injurious to the skin. Vancouver, BC: Greenglass Ltd.; 1979.

8. Northeastern Lumber Manufacturers Association. Northeastern white pine, its grades and uses. New York, NY, USA.: NLMA; 1950.

9. Record, S. J. and Hess R. W. Timbers of the new world. New Haven, CT: Yale University Press; 1943.

10. Simpson, W. T. Dry kiln operator's manual. Madison, WI: USDA Forest Service, FPL Ag. Handbook No. 188; 1991.

11. Summitt, R. and Sliker, A. CRC handbook of materials science. Vol. 4. Boca Raton, FL: CRC Press, Inc.; 1980.

12. USDA. Wood handbook: wood as an engineering material. Madison, WI: USDA Forest Service, FPL Ag. Handbook No. 72;

1974.

13. Wendel, G. W. and Smith, H. C. Pinus strobus L. Eastern White Pine. in: Burns, R. M. and Honkala, B. H., tech. coords. Silvics of North America. Volume 1, Conifers. Washington, DC: USDA Forest Service; 1990; pp. 476-488.

14. Woods, B. and Calnan, C. D. Toxic woods. British Journal of Dermatology. 1976; 95(13):1-