Pinus elliottii Engelm.

 

 

click here for the page in Engilsh units of measure

this page uses metric units of measure

 

Family: Pinaceae

 

 

 

 

 

 

click to print or download the file in .pdf format

 

Slash Pine

 

 

 

 

The genus Pinus is composed of about 95 species native to temperate and tropical regions of the world. There are 60 species in the New World (North America and South America) and 35 in the Old World (Eurasia and northern Africa). In the New World, there are 4 native to the West Indies, 5 in Central America, 38 in Mexico and 37 in the United States and Canada. The wood of pine can be separated microscopically into the white, red, yellow and the foxtail/pinyon pine groups. Slash pine is in the yellow pine group. The word pinus is the classical Latin name and elliottii is used in honor of Stephen Elliott (1771-1830), botanist and banker of South Carolina and author of "Sketch of the Botany of South-Carolina and Georgia". Slash pine has two recognized varieties, the typical slash pine (Pinus elliottii Engelm. var. elliotti) and South Florida slash pine (Pinus elliottii var densa Little & Dorman).

Other Common Names: American pitch pine, bastard pine, British Honduras pitch pine, Cuba pine, Dade County pine, Dade County slash pine, Ellotti-tall, Florida pine, Florida southern pine, Florida-tall, Gulf Coast pitch pine, longleaf, longleaf pine, longleaf pitch pine, longleaf yellow pine, meadow pine, Nicaraguan pine, pin de la Floride du sud, pinavete, pino de Florida del sur, pino di Florida del sud, pino grasso, pino pece, pino tea, pitch pine, pitchpin Americain, saltwater pine, she pine, South Florida slash pine, Southern Florida pine, southern Florida slash pine, southern pine, southern yellow pine, spruce pine, swamp pine, thong, yellow pine, yellow slash pine, Zuid-Florida pijn.

Distribution: Slash pine is native to the coastal plains from southern South Carolina to southern Florida (also the lower Florida Keys), west to southeast Louisiana.

The Tree: Slash pine trees reach heights of 70 feet (21.34 m) with a 2 foot (0.61 m) diameter.

General Wood Characteristics: The sapwood of slash pine is a yellowish white, while the heartwood is a reddish brown. It is very strong and heavy, very stiff, hard and moderately high in shock resistance. It has straight grain, is medium in texture and relatively difficult to work with hand tools. It ranks high in nail holding capacity, but is difficult to glue.

 

Mechanical Properties (2-inch standard)

 

 

 

 

Compression

 

 

 

 

Specific

Gravity

MOE

GPa

MOR

MPa

Parallel

MPa

Perpendicular

MPa

WMLa

KJ/m3

Hardness

N

Shear

MPa

Green

0.54

10.5

60.0

26.3

3.65

66.2

NA

6.62

Dry

0.66

13.6

112

56.1

7.03

91.0

NA

11.58

aWML = Work to maximum load.

Reference (56).

 

Drying and Shrinkage

Type of shrinkage

Percentage of shrinkage
(green to final moisture content)

0% MC

6% MC

20% MC

Tangential

7.6

6.2

2.6

Radial

5.4

4.4

1.8

Volumetric

12.1

9.8

4.1

References: (185, 56, 192).

Kiln Drying Schedulesa

 

Conventional temperature/moisture content-controlled schedulesa


Condition

4/4, 5/4
stock

6/4 stock

8/4
stock

10/4
stock

12/4
stock

British schedule
4/4 stock

Standard

T13-C6

T12-C5

T12-C5

T10-C4

T10-C4

L

Highest Quality

279

279

279

T10-C4

T10-C4

NA

aReference (28, 185).

 

Conventional temperature/time-controlled schedulesa

 

Lower grades

Upper grades


Condition

4/4, 5/4 stock

6/4 stock

8/4 stock

4/4, 5/4 stock

6/4 stock

8/4 stock

12/4, 16/4 stock

Standard

281

NA

282

281

NA

282

284

aReferences (28, 185).

 

High temperaturea


Condition

4/4, 5/4 stock

6/4 stock

8/4 stock


Other products

Standard

401/402

NA

NA

403 (2 by 4's)

aReferences (28, 185).

 

 

Working Properties: Slash pine is difficult to work with hand tools, but ranks high in nail holding capacity.

Durability: It is rated as moderately resistant to heartwood decay (187).

Preservation: The sapwood is easy to impregnate with preservatives, while the heartwood is difficult. Pressure treatments may extend durability and usefulness considerably.

Uses: The wood is used for heavy construction (bridges, trestles and dock works), pulp, plywood, utility poles, piling, railroad ties, mine timbers. The sap is used for rosin and turpentine.

Toxicity: In general, working with pine wood may cause dermatitis, allergic bronchial asthma or rhinitis in some individuals (69, 150 & 207).

 

Additional Reading and References Cited (in parentheses)

28. Boone, R. S.; Kozlik, C. J.; Bois, P. J., and Wengert, E. M. Dry kiln schedules for commercial woods - temperate and tropical. Madison, WI: USDA Forest Service, FPL-GTR-57; 1988.

58. Gaby, L. I. The southern pines, an American wood. Washington, DC, USA: USDA Forest Service, FS-256; 1985.

69. Hausen, B. M. Woods injurious to human health. A manual. New York, NY: Walter de Gruyter; 1981.

72. Henderson, F. Y. A handbook of softwoods. London: HMSO; 1977.

75. Hyam, R. and Pankhurst, R. Plant and their names. A concise dictionary. Oxford, UK: Oxford University Press; 1995.

109. ---. Checklist of United States Trees (Native and Naturalized). Washington, D.C.: U.S. Government Printing Office, USDA, Forest Service, Agriculture Handbook No. 541; 1979.

133. Lohrey, R. E. and Kossuth, S. V. Pinus elliottii Engelm. Slash Pine. in: Burns, R. M. and Honkala, B. H., tech. coords. Silvics of North America. Volume 1, Conifers. Washington, DC: USDA Forest Service; 1990; pp. 338-347.

150. Mitchell, J. and Rook, A. Botanical dermatology: plants and plant products injurious to the skin. Vancouver, BC: Greenglass Ltd.; 1979.

163. Record, S. J. and Hess R. W. Timbers of the new world. New Haven, CT: Yale University Press; 1943.

177. Simpson, W. T. Dry kiln operator's manual. Madison, WI: USDA Forest Service, FPL Ag. Handbook No. 188; 1991.

184. Summitt, R. and Sliker, A. CRC handbook of materials science. Vol. 4. Boca Raton, FL: CRC Press, Inc.; 1980.

187. USDA. Wood handbook: wood as an engineering material. Madison, WI: USDA Forest Service, FPL Ag. Handbook No. 72; 1974.

207. Woods, B. and Calnan, C. D. Toxic woods. British Journal of Dermatology. 1976; 95(13):1-97.